Crucible steel is steel made by melting pig iron, cast iron, iron, and sometimes steel, often along with sand, glass, ashes, and other fluxes, in a crucible. Crucible steel was first developed in the middle of the 1st millennium BCE in Southern India and Sri Lanka using the wootz process.
In pre-industrial times, it was not possible to produce sufficient temperatures with charcoal or coal fires required to melt iron or steel. However, pig iron, having a higher net alloy content and thus a lower melting point, could be melted. This is due to the effect of Freezing Point Depression. By co-heating wrought iron or steel with pig-iron for a long time, Carbon content in the pig iron could be reduced as it slowly diffused into the iron. In addition, H2O containing organic materials could be mixed into fluxing agents. Oxygen reacted with excess phosphorus, sulfur, and silicon typical of pig iron producing additional heat and low density slag. The additional heat was sufficient to dissolve some or all of Wrought Iron scraps turning the previous raw materials into a medium-carbon steel ingot. This also allowed slag and oxide inclusions in the W.I. to float on the surface, producing superior internal cleanliness. Crucible steel of this type was produced in South and Central Asia during the medieval era.
This generally produced a very hard steel, but also an ingot that might be inhomogeneous, consisting of a very high-carbon steel regions (formerly the pig-iron) and lower-carbon steel regions (formerly the wrought iron).
The crucible steel process might result in an intricate pattern when the steel was filed, polished, then etched. Possibly the most well-known examples coming from the wootz steel used in Damascus swords. Such steel was typically higher in average carbon content (typically ranging in the area of 1.5 to 2.0%) and relatively high in phosphorus, which contributed to the distinctive water pattern. This effect was caused by slowly cooling the cruicibles over several days.
The preceding factors caused an excessively coarse, dendritic crystal grain structure in crucible steel ingots, and alloy segregation at the edges of the grains as they grew. The increased alloy content at the as-cooled grain boundaries caused the steel to be attacked more slowly by etchants, resulting in a frost-like or woodgrain-like pattern after polishing and etching. However the majority of crucible steel ingots did not exhibit this effect. This led items showing the effect to be ascribed mystical properties. Although it was merely a result of excessively coarse grain size and a particular alloy composition.
The steel was usually subjected to a grain refinement heat treatment, then forged at relatively low temperatures to avoid hot-shortness, crumbling, or excess diffusion of carbon.
With a carbon content close to that of cast iron, it usually required minimal heat treatment after finishing other than air cooling amd tempering to achieve the correct hardness, relying on composition alone.
In Europe, crucible steel was developed in parallel during the 1740s, by Benjamin Huntsman, of Sheffield, England. Huntsman used coke, rather than charcoal, achieving temperatures high enough to melt steel and dissolve iron, in combination with a glass shard flux to reduce impurities. Huntsman's process differed from some of the Wootz processes in that it used iron and steel as raw materials, in the form of blister steel, rather than direct conversion from cast iron as in puddling or the later Bessemer process, a glass flux to reduce impurities, and the higher temperatures and carbon content of coke, along with a longer time to melt the steel and to cool it down, to thus allowed more time for the diffusion of carbon.
The ability to fully melt the steel removed any inhomogeneities in the steel, allowing the carbon to dissolve evenly into the liquid steel and negating the prior need for extensive blacksmithing in an attempt to achieve the same result. Similarly, it allowed steel to be cast by pouring into molds. The use of fluxes allowed nearly complete extraction of impurities from the liquid, which could then simply float to the top for removal. This produced the first steel of modern quality, providing a means of efficiently changing excess wrought iron into useful steel. Huntsman's process greatly increased the European output of quality steel suitable for use in items like knives, tools, and machinery, helping to pave the way for the Industrial Revolution.